査読付き雑誌論文の一覧へ戻るBack to Peer-reviewed journal papers
Application Phase Analysis for Predicting High-Speed Crack Propagation/Arrest in 3D Thick Plates Using S-version FEM
- 著者Authors
- T. He, N. Morita, N. Mitsume, F. Yanagimoto, K. Suzuki, Y. J. Kim, K. Shibanuma†
- 掲載先Published in
- Engineering Fracture Mechanics
- 巻号、ページVolume, pages
- Vol.322, p.111173
- 年Year
- 2025
- 種類Type
- 査読付き雑誌論文Peer-reviewed journal papers
- Link
- https://doi.org/10.1016/j.engfracmech.2025.111173
- 研究テーマTopics
- 有限要素法Finite element method 破壊力学Fracture mechanics 構造・固体Structural and solid mechanics 波・海洋Waves and ocean engineering
- キーワードKeywords
- Application phase 解析Application phase analysis 高速亀裂伝播High-speed crack propagation 亀裂停止Crack arrest 3 次元厚板3D thick plate 重合メッシュ法S-version finite element method 破壊力学Fracture mechanics 3 次元の高速亀裂伝播の予測3D high-speed crack propagation prediction PMMA(ポリメタクリル酸メチル)PMMA 最適化アルゴリズムOptimisation algorithm 亀裂停止長さCrack arrest length
概要
厚板は船舶、タンク、パイプラインなどの大規模な構造物に広く使われ、脆性亀裂の高速伝播はその安全性に関わる重大な問題です。脆性破壊の発生を完全に防ぐことは難しいため、厚板の中を進む亀裂の伝播と停止を精度よく予測することが、破壊を制御するために欠かせません。
高速亀裂の数値解析には、実験で得た亀裂の履歴を入力として応力場や動的応力拡大係数を求める Generation phase 解析(順解析)と、亀裂の伝播条件と停止条件を入力として亀裂の挙動を予測する Application phase 解析(逆解析)があります。著者らはこれまで重合メッシュ法(S-version FEM)を使って Generation phase 解析を発展させてきましたが、3 次元構造の高速亀裂の伝播と停止を予測する Application phase 解析の手法は確立されていませんでした。
本論文は、重合メッシュ法に基づく動的亀裂伝播モデルを使い、3 次元の厚板を対象に、高速亀裂の伝播と停止を予測する Application phase 解析の手法を提案しています(論文は、このような手法は初めてであると述べています)。解析は、亀裂発生後の安定な伝播を扱う Segment I と、その後の高速伝播から停止までを扱う Segment II からなり、どちらの区間でも、非線形勾配降下法と黄金分割法を組み合わせた最適化によって、各ステップの亀裂速度と亀裂前縁形状を定めます。
ポリメタクリル酸メチル(PMMA)製の二重片持ち梁(DCB)型試験片を使った 5 回の亀裂停止試験と比較した結果、論文は、試験片の振動が原因と考えられる亀裂速度の振動まで含めて亀裂の挙動を再現でき、亀裂停止長さの正規化誤差の最大値は 10 % 未満であったと報告しています。
重要点
1. 逆解析(Application phase 解析)によって、3 次元の高速亀裂の伝播と停止を予測する
高速亀裂の数値解析には 2 つの方向があります(図 1)。Generation phase 解析は順解析で、亀裂の発生から停止までの亀裂速度の履歴と亀裂前縁形状の履歴を明示的な入力とし、各ステップの有限要素解析(FEA)で応力場と動的応力拡大係数(DSIF)を求めて、亀裂伝播条件と材料定数を定めます。Application phase 解析は逆解析で、亀裂伝播条件と亀裂停止条件を入力とします。各ステップの開始時には FEA に必要な亀裂の挙動が未知なので、最適化によって FEA を繰り返し、亀裂伝播条件を満たす亀裂速度と亀裂前縁形状を定めます。
論文によれば、Application phase 解析の従来の研究の多くは 2 次元モデルで、亀裂前縁の形状を考慮しておらず、破壊パラメータが単一の値になるため、実構造の問題には適していません。3 次元の亀裂伝播を予測した研究もありますが、実構造の健全性の確保で重要な亀裂停止の予測を扱っていません。本論文は、3 次元構造の高速亀裂の伝播と停止を予測する Application phase 解析の手法を初めて提案すると述べています。研究の目的は、亀裂停止長さと負荷条件の 1 対 1 の関係を予測することで、亀裂発生の予測は対象に含めていません。
2. 重合メッシュ法により、ローカルメッシュの更新だけで亀裂前縁の変化を表す
有限要素解析には、著者らの先行研究の重合メッシュ法(S-version FEM、論文の略称は s-method)に基づく動的亀裂伝播モデルを使っています。重合メッシュ法は、粗いグローバルメッシュで構造全体を、細かいローカルメッシュで亀裂前縁の周りを表す方法で、ローカルメッシュの領域では両方のメッシュの解を足し合わせて変位と加速度を表します。ローカルメッシュは構造の形状とは独立に定義でき、亀裂の進展と最適化の反復に合わせて更新しますが、グローバルメッシュは解析の間ずっと変えません(図 2)。論文は、これにより最適化の処理をローカルメッシュの領域だけに集中でき、アルゴリズムが単純になると述べています。また、ローカルメッシュは亀裂前縁を覆うために板の表面の外まで延びるので、板の表面(表面力のない境界)の表現にはヘビサイド関数によるエンリッチメントを併用しています。
亀裂前縁の形状は板厚方向に対称と仮定し(解析モデルは全体の 1/4)、次の 2 次関数で近似します。
ここで、 は亀裂が進む方向の座標、 は板厚方向の座標(板厚の中央で )、 は亀裂前縁の最も深い点(板厚の中央の亀裂先端)の 座標、 は亀裂前縁の形を表すパラメータです。Application phase 解析では、板厚中央の亀裂速度 と の 2 つが、各ステップで求める未知量になります。

3. 亀裂の伝播条件と停止条件を定式化する
亀裂の伝播中は、駆動力である動的応力拡大係数 と、亀裂速度 の関数である材料抵抗 が釣り合います。
ただし、亀裂前縁を 2 次関数で近似しているので、前縁のすべての節点で式 (52) を厳密に満たすことは難しいと論文は述べています。そこで、亀裂伝播条件を次の目的関数の最小化によって定義します。
ここで、 は目的関数、 は、 と を定数 と で割って正規化した値(、、原論文の式 (53)、(54))を並べたパラメータベクトル、 は亀裂前縁上のローカルメッシュの節点の数、 は亀裂前縁の 番目の節点の動的応力拡大係数、 は亀裂前縁に沿った亀裂速度です。亀裂伝播条件は、反復の番号を 、第 反復のパラメータベクトルを 、許容値を として、次の式が成り立つことです。
亀裂の停止は、亀裂前縁に沿って正の亀裂速度を与える解がなくなることとして定義しています。亀裂前縁を 2 次関数で近似しているので、判定は板厚の中央と板の表面の 2 点で行います。板厚の中央では (原論文の式 (57))、板の表面では、表面の亀裂速度の式(原論文の式 (58))の分子が負になることを調べます。
ここで、 は板厚の半分、 はステップ の亀裂先端の 座標、 と はステップ と の亀裂前縁の形を表すパラメータです。板厚の中央または板の表面の亀裂速度が負になると、亀裂が停止したと判定します。
4. Segment I と Segment II の 2 区間と、勾配降下法と黄金分割法を組み合わせた最適化
解析は 2 つの区間からなります(図 3)。Segment I は、亀裂発生後の安定な亀裂伝播(ステップ 1 から まで。本論文では )を解析します。この区間では DSIF をステップ でだけ評価するので、亀裂の挙動は区間全体で一定と仮定します。Segment II は、ステップ から亀裂の停止までの各ステップで、亀裂の挙動をステップごとに定めます。論文は、この分割によって亀裂発生の計算コストの大きい解析が不要になり、Segment II の出発点が定まって最適化の反復回数が減ると述べています。

どちらの区間でも、最適化は 2 段階で行います。第 1 段階では、非線形勾配降下法で最適化の方向を定めます。目的関数の勾配は、パラメータを微小量だけ変えた 2 回の追加の FEA から、次のように差分で計算します。
ここで、 と は微小量で、、 です。第 2 段階では、黄金分割法で最適化のステップ長を定めます(原論文の式 (61)〜(64))。こうして更新したパラメータベクトル で FEA を行い、式 (56) が成り立つまで繰り返します。Segment II では、各ステップの収束の後に亀裂停止条件を調べ、亀裂が停止していなければ次のステップに進みます。
数値実験の結果
PMMA 厚板の DCB 型亀裂停止試験(5 試験)
透明なポリメタクリル酸メチル(PMMA)の厚板で作った二重片持ち梁(DCB)型試験片の亀裂停止試験 5 回(P1〜P5)と比較して、提案手法を検証しています。試験片は高さ 180 mm、幅 110 mm、板厚 30 mm で、切欠きの先端(半径 は 0.8、1.0、1.2 mm の 3 種類)の位置を とします(図 4)。材料はヤング率 3,200 MPa、ポアソン比 0.35、密度 1,170 kg/m³ です(原論文 Table 1)。室温 20 ℃ の準静的な負荷でくさびによってピンを押し広げて亀裂を発生させ、亀裂前縁の動きを高速度カメラ(毎秒 300,000 コマ)で撮影しました。実験の結果は次のとおりです(原論文 Table 2。 はクリップゲージ開口変位、 は亀裂前縁の最も深い点で測った亀裂停止長さ)。
| 試験片 | 切欠きの半径 [mm] | クリップゲージ開口変位 [mm] | 亀裂停止長さ [mm] |
|---|---|---|---|
| P1 | 0.8 | 0.326 | 88.1 |
| P2 | 1.0 | 0.324 | 80.3 |
| P3 | 0.8 | 0.234 | 51.3 |
| P4 | 1.2 | 0.442 | 116.8 |
| P5 | 1.2 | 0.397 | 103.1 |
解析は 1/4 対称モデルで行い、ローカルメッシュの要素の大きさは、亀裂が進む方向とその法線方向に 0.300 mm、亀裂前縁の方向に 0.600 mm です(原論文 Table 3)。ピンの穴はモデルから省き、実験のクリップゲージ開口変位に合うように静的解析で定めたピン開口変位を、一定の負荷条件として与えています(原論文 Table 4)。亀裂伝播条件の材料抵抗 は、試験 P1 と P2 の結果を用いた Generation phase 解析から定めた近似式(原論文の式 (D.1))です。
図 5 は、試験 P2 と P3 の 対称面(亀裂の面)の応力 (亀裂の面に垂直な方向の応力)の分布の予測を、高速度カメラの写真と比べたものです。亀裂の発生から停止までの現象全体は 0.001 秒未満で終わると論文は述べています。
図 6 は、5 試験の亀裂速度の履歴を実験と比べたものです。論文は、提案手法が亀裂速度の全体的な履歴だけでなく、実験で見られた亀裂速度の振動(試験片の振動によるものと考えられる)も再現したと述べています。

図 7 は、亀裂停止長さの予測と実験の比較です。論文によれば、亀裂停止長さの正規化誤差の最大値は 10 % 未満で、短い亀裂から長い亀裂までを同じ手法で扱えることを示しています。正規化誤差は、実験と予測の亀裂停止長さの差を、試験片の高さから切欠きの長さを引いた値で割ったものです。論文は、実験との差の原因として、材料抵抗の定式化の簡略化(DSIF が亀裂速度だけに依存すると仮定していること)と、実験の不確かさ(特に試験 P4 と P5 の亀裂前縁の対称性)を挙げています。
今後の展開
論文は、予測精度を高めるための今後の課題として、材料抵抗の定式化に亀裂の加速度と応力三軸度を取り入れることと、シェブロン形の切欠きを用いて亀裂前縁の対称性を高めるように実験を改善することを挙げています。また、亀裂伝播条件の基礎は材料に応じて変えられるとして、鋼の脆性亀裂には局所破壊応力、高圧ガスパイプラインの亀裂には亀裂先端開口角(CTOA)を用いる例を挙げています。
Overview
Thick plates are widely used in large structures such as ships, tanks and pipelines, and the high-speed propagation of brittle cracks in these plates is a serious safety issue. Because it is difficult to prevent brittle fracture from initiating completely, accurately predicting the propagation and arrest of cracks running through thick plates is essential for controlling fracture.
Numerical analysis of high-speed cracks has two directions: generation phase analysis (a forward analysis), which takes experimentally obtained crack histories as inputs and evaluates stress fields and dynamic stress intensity factors, and application phase analysis (an inverse analysis), which takes crack propagation and arrest conditions as inputs and predicts the crack behaviour. The authors have advanced generation phase analysis using the S-version finite element method (S-version FEM), but a strategy for application phase analysis that predicts high-speed crack propagation and arrest in 3D structures had not been established.
This paper proposes such a strategy for three-dimensional thick plates, based on a dynamic crack propagation model using the S-version FEM (the paper states that this is the first such strategy). The analysis consists of Segment I, which treats the stable propagation after crack initiation, and Segment II, which treats the subsequent high-speed propagation up to arrest; in both segments, an optimisation algorithm combining the Non-linear Gradient Descent and Golden Section methods determines the crack velocity and crack-front shape at each step.
Based on a comparison with five crack arrest tests using double cantilever beam (DCB)-type specimens made of polymethyl methacrylate (PMMA), the paper reports that the crack behaviour is reproduced, including the crack velocity oscillations likely caused by specimen vibrations, and that the maximum normalised error in crack arrest length is less than 10 %.
Key points
1. Predicting high-speed crack propagation and arrest in 3D by inverse analysis (application phase analysis)
Numerical analysis of high-speed cracks has two directions (Figure 1). Generation phase analysis is a forward analysis: it takes the histories of crack velocity and crack-front shape from initiation to arrest as explicit inputs, performs a finite element analysis (FEA) at each step to obtain stress fields and dynamic stress intensity factors (DSIFs), and thereby determines the crack propagation conditions and material constants. Application phase analysis is an inverse analysis that takes the crack propagation and arrest conditions as inputs. At the beginning of each step, the crack behaviour needed for the FEA is unknown, so the FEA is repeated within an optimisation to find the crack velocity and crack-front shape that satisfy the crack propagation condition.
According to the paper, most previous studies of application phase analysis used 2D models, which do not account for the crack-front shape and reduce the fracture parameter to a single value, making them unsuitable for real-world structures. Some studies predicted crack propagation in 3D, but they did not address the prediction of crack arrest, which is important for ensuring the integrity of actual structures. The paper states that it proposes the first strategy for application phase analysis that predicts high-speed crack propagation and arrest in 3D structures. The objective is to predict a one-to-one relationship between crack arrest length and loading conditions; predicting crack initiation is outside the scope.

2. With the S-version FEM, changes of the crack front are represented by updating only the local mesh
The FEA uses the dynamic crack propagation model based on the S-version finite element method (S-version FEM, abbreviated in the paper as the s-method) from the authors' previous work. The method represents the whole structure with a coarse global mesh and the region around the crack front with a fine local mesh, and in the local-mesh domain the displacement and acceleration are expressed by adding the solutions of the two meshes. The local mesh can be defined independently of the structural geometry and is updated with crack propagation and the optimisation iterations, while the global mesh is kept unchanged throughout the analysis (Figure 2). The paper states that this allows the optimisation process to focus only on the local domain, which simplifies the algorithm. In addition, because the local mesh extends beyond the plate surfaces to cover the crack front, Heaviside enrichment is used together with it to represent the plate surfaces (traction-free boundaries).
The crack-front shape is assumed to be symmetric in the thickness direction (the analysis model is one quarter of the whole) and is approximated by the following quadratic function.
Here, is the coordinate in the crack propagation direction, is the coordinate in the thickness direction ( at the mid-thickness), is the -coordinate of the deepest point of the crack front (the crack tip at the mid-thickness), and is the parameter describing the crack-front shape. In the application phase analysis, the crack velocity at the mid-thickness, , and are the two unknowns determined at each step.

3. Formulating the crack propagation and arrest conditions
During crack propagation, the driving force, the dynamic stress intensity factor , is in equilibrium with the material resistance , which is a function of the crack velocity .
However, because the crack front is approximated by a quadratic function, the paper notes that it is difficult to satisfy Eq. (52) exactly at every node on the crack front. The crack propagation condition is therefore defined through the minimisation of the following objective function.
Here, is the objective function, is the parameter vector consisting of and normalised by the constants and (, ; Eqs. (53) and (54) of the original paper), is the number of local-mesh nodes on the crack front, is the dynamic stress intensity factor at the -th node on the crack front, and is the crack velocity along the crack front. The crack propagation condition is that the following inequality holds, where is the iteration number, is the parameter vector at the -th iteration, and is the tolerance.
Crack arrest is defined as the absence of a solution that gives a positive crack velocity along the crack front. Because the crack front is approximated by a quadratic function, the assessment is made at two points only, the mid-thickness and the plate surface. At the mid-thickness, the condition is (Eq. (57) of the original paper); at the plate surface, it is checked whether the numerator of the expression for the crack velocity at the surface (Eq. (58) of the original paper) is negative.
Here, is the half-thickness of the plate, is the -coordinate of the crack tip at step , and and are the parameters describing the crack-front shape at steps and . The crack is judged to have arrested when the crack velocity at either the mid-thickness or the plate surface becomes negative.
4. Two segments, Segment I and Segment II, and an optimisation combining gradient descent and the golden section method
The analysis consists of two segments (Figure 3). Segment I analyses the stable crack propagation after initiation (from step 1 to step ; in this paper). In this segment, the DSIF is evaluated only at step , so the crack behaviour is assumed to be constant over the segment. Segment II determines the crack behaviour individually for each step from step until crack arrest. The paper states that this division eliminates the need for computationally expensive simulations of crack initiation and provides a starting point for Segment II that reduces the number of optimisation iterations.

In both segments, the optimisation is performed in two stages. In the first stage, the Non-linear Gradient Descent method determines the optimisation direction. The gradient of the objective function is computed by differences from two additional FEAs in which the parameters are changed by minute values.
Here, and are minute values, with and . In the second stage, the Golden Section method determines the optimisation step length (Eqs. (61) to (64) of the original paper). The FEA is then performed with the updated parameter vector , and the procedure is repeated until Eq. (56) holds. In Segment II, the crack arrest condition is assessed after each step has converged, and the analysis proceeds to the next step if the crack has not arrested.
Numerical results
DCB-type crack arrest tests on thick PMMA plates (five tests)
The proposed strategy is validated against five crack arrest tests (P1 to P5) on double cantilever beam (DCB)-type specimens made of transparent polymethyl methacrylate (PMMA) thick plates. The specimens are 180 mm high, 110 mm wide and 30 mm thick, and the notch root (with a radius of 0.8, 1.0 or 1.2 mm) is located at (Figure 4). The material has a Young's modulus of 3,200 MPa, a Poisson's ratio of 0.35 and a density of 1,170 kg/m³ (Table 1 of the original paper). The cracks were initiated by separating the pins with wedges under quasi-static loading at a room temperature of 20 ℃, and the motion of the crack front was captured with a high-speed camera (300,000 frames per second). The experimental results are as follows (Table 2 of the original paper; is the clip gauge opening displacement, and is the crack arrest length measured at the deepest point of the crack front).
| Specimen | Notch radius [mm] | Clip gauge opening displacement [mm] | Crack arrest length [mm] |
|---|---|---|---|
| P1 | 0.8 | 0.326 | 88.1 |
| P2 | 1.0 | 0.324 | 80.3 |
| P3 | 0.8 | 0.234 | 51.3 |
| P4 | 1.2 | 0.442 | 116.8 |
| P5 | 1.2 | 0.397 | 103.1 |

The analysis uses a quarter-symmetric model, and the local-mesh element size is 0.300 mm in the crack propagation direction and its normal direction and 0.600 mm along the crack front (Table 3 of the original paper). The pinholes are omitted from the model; the pin opening displacement, determined by static analysis to match the experimental clip gauge opening displacement, is applied as a constant loading condition (Table 4 of the original paper). The material resistance in the crack propagation condition is an approximation (Eq. (D.1) of the original paper) determined from generation phase analysis using the results of tests P1 and P2.
Figure 5 compares the predicted distributions of the stress (the stress normal to the crack plane) on the -symmetric plane (the crack plane) for tests P2 and P3 with high-speed camera photographs. The paper states that the entire phenomenon from crack initiation to arrest takes place in less than 0.001 s.

Figure 6 compares the predicted histories of crack velocity with the experiments for the five tests. The paper states that the proposed strategy reproduces not only the overall history of crack velocity but also the crack velocity oscillations observed in the experiments (which may be attributed to specimen vibrations).

Figure 7 compares the predicted and experimental crack arrest lengths. According to the paper, the maximum normalised error in crack arrest length is less than 10 %, which shows that the strategy can handle both short and long cracks. The normalised error is the difference between the experimental and predicted crack arrest lengths divided by the specimen height minus the notch length. The paper attributes the discrepancies to the simplification of the material resistance formulation (assuming that the DSIF depends only on crack velocity) and to experimental uncertainties (in particular, the crack-front symmetry in tests P4 and P5).

Outlook
As future work to improve the predictive accuracy, the paper mentions incorporating crack acceleration and stress triaxiality into the material resistance formulation and improving the experiments by using chevron-shaped notches to achieve better crack-front symmetry. The paper also states that the basis of the crack propagation condition can be changed according to the material, giving as examples the local fracture stress for brittle crack propagation in steel and the crack tip opening angle (CTOA) for crack propagation in high-pressure gas pipelines.